日本在线www-日本在线播放一区-日本在线不卡免费视频一区-日本在线不卡视频-成人影院久久久久久影院-成人影院一区二区三区

Causes and solutions for the brittleness of PVC plastic prof
欄目:Industry News 發布時間:2021-06-03 15:19
Second, the extrusion process is unreasonable 1. Excessive or insufficient plasticization of materials This is related to the process temperature setting and feed ratio. If the temperature is set too high, the material will be over-plasticiz...
Second, the extrusion process is unreasonable
1. Excessive or insufficient plasticization of materials
This is related to the process temperature setting and feed ratio. If the temperature is set too high, the material will be over-plasticized. Some lower molecular weight components will decompose and volatilize. If the temperature is too low, there will be no molecules between the components.
Completely fused, the molecular structure is not strong.
However, if the feed ratio is too large, the heated area and shearing force of the material increase, the pressure increases, and it is easy to cause excessive plasticization; if the feed ratio is too small, the heating area and shearing force of the material will decrease, which will Causes less plasticization.
Whether it is excessive plasticization or superplasticization, it will lead to the cutting and folding of profiles.
2, insufficient head pressure
On the one hand, it is related to the mold design (this will be described separately below). On the other hand, it is related to the feed ratio and temperature setting. When the pressure is insufficient, the compactness of the material is poor and the looseness of the material appears to be loose.
The metering feed rate and the extrusion screw speed should be adjusted to control the pressure between 25 MPa and 35 MPa.
3. The low molecular components in the product are not discharged.
There are generally two ways to produce low molecular weight components in the product, one that is produced during the hot mixing process and can be discharged through the dehumidification and exhaust system during hot mixing.
The second is partially residual and heated water and hydrogen chloride gas generated during heating.
This is usually forced out through a forced exhaust system in the exhaust section of the main engine. The vacuum is usually between -0.05 MPa and 0.08 MPa. If it is not opened or too low, low molecular components will remain in the product, resulting in a decrease in the mechanical properties of the profile.
4, the screw torque is too low
The torque of the screw is the value of the reaction machine under force. Set the value of the process temperature. The feed ratio is directly reflected in the screw torque value. The screw torque is too low to be reflected to some extent.
The temperature is low or the feed ratio is small, so the material is not completely plasticized to the extent of extrusion and the mechanical properties of the profile are also reduced.
Depending on the extrusion equipment and mold, the screw torque is typically between 60% and 85% to meet the requirements.
5. The traction speed does not match the extrusion speed.
If the pulling speed is too fast, the mechanical properties of the profile wall will be reduced and the pulling speed will be too slow. The resistance of the profile is large and the product is in a high tensile state, which also affects the mechanical properties of the profile.
Third, the mold design is not reasonable
1. The design of the mold part is unreasonable, especially the distribution of the inner ribs and the treatment of the interface angle.
This can lead to stress concentrations, and it is necessary to improve the design and eliminate the right and acute angles at the interface.
2. The mold pressure is insufficient.
The pressure of the mold is directly dependent on the compression ratio of the mold, especially the length of the straight section of the mold.
If the compression ratio of the mold is too small or the straight portion is too short, the product will not be dense and affect physical properties.
On the one hand, the change in mold pressure can be adjusted by changing the length of the flat portion of the mold; on the other hand, different compression ratios can be selected to change the extrusion pressure at the mold design stage, but attention must be paid to the compression ratio of the indenter.
The compression ratio of the extruder screw is adapted; the extrusion process parameters can also be adjusted and the porosity can be increased by changing the formulation.
The plate changes the amount of melt pressure.
3. For performance degradation caused by poor convergence of the split ribs, the length of the ribs and the outer surface, the ribs and ribs at the confluence should be appropriately increased, or the compression ratio should be increased to solve.
4. The mold discharge is uneven, resulting in inconsistent wall thickness or inconsistent profiles.
This also results in a difference in mechanical properties between the two faces of the profile. We sometimes failed to pass the test when we were cold, which proves this.
As for non-standard profiles such as thin walls, we will not repeat them here.
5. The cooling rate of the sizing die.
The cooling water temperature usually does not cause enough attention. The function of the cooling water is to cool and shape the macromolecular chain of the profile in time for the purpose of use.
Slow cooling allows the molecular chain to extend for a sufficient time to promote shaping.
Rapid cooling, the temperature difference between the water temperature and the extruded parison is too large, and the product is quenched, which is not conducive to the improvement of the low temperature performance of the product.
From the explanation of polymer physics, PVC macromolecular chains undergo crimping and stretching under the action of temperature and external force. When the temperature and external force are taken out, the macromolecular chain does not recover in a free state and is out of the glass state.
The disordered arrangement of chains leads to low temperature impact properties of macroscopic products.
From
Plastic processing techniques explain the existence of a stress relaxation process after removal of the PVC profile after removal of the product from temperature and external forces.
A suitable cooling water temperature is beneficial to the process.
When the temperature of the cooling water is too low, the stress in the product does not disappear, resulting in a decrease in product performance. Therefore, the profile cooling is slowly cooled, and warpage, bending, and shrinkage of the molded product can be prevented, and the impact strength of the product can be prevented from being lowered due to internal stress.
Usually, the water temperature is controlled at 20 °C.
In order to gently cool the parison without quenching, the water pipe connected to the cooling sizing sleeve is connected to the rear of the molding so that the flow direction of the water in the sizing sleeve is opposite to the moving direction. The front part is discharged.
This does not cause the parison to be quenched due to low water temperature, excessive internal stress, and the profile is fragile, and the impact resistance of the profile is lowered. (to be continued)
全免费A级毛片免费看视频| 亚洲AⅤ优女AV综合久久久 | 国产成人亚洲综合无码18禁禁| 综合无码成人AⅤ视频在线观看| 亚洲欧美偷拍另类A∨| 无码欧精品亚洲日韩一区| 日韩精品一区二区亚洲AV| 女神被啪进深处娇喘在线观看| 久久精品国产清自在天天线 | 蜜桃视频一区二区| 久久AV无码专区亚洲AV桃花岛| 国产又色又爽又黄的网站在线| 国产精品成人免费视频网站| 丰满的少妇愉情HD高清免费 | 成人片黄网站色大片免费观看| Chinese老妇性饥渴老熟女| 重囗味SM在线观看无码| 中国熟妇人妻XXXXX中文| 尹人香蕉久久99天天拍| 一个添下面两个吃奶| 亚洲一区二区自偷自拍另类| 亚洲精品无码日韩国产不卡Av| 亚洲AV无码专区在线电影成人网| 性色生活片在线观看| 性一交一乱一色一视频| 性欧美长视频免费观看不卡 | 亚洲AV无码一区二区三区天堂古| 五月丁香六月缴情基地| 午夜成人无码片在线观看影院| 无码国产伦一区二区三区视频| 天黑黑影院免费观看视频在线播放| 少妇私密会所按摩到高潮呻吟| 色综合精品无码一区二区三区| 日韩成人无码AV| 色综合色综合久久综合频道88| 少妇激情A∨一区二区三区| 少妇呻吟翘臀后进爆白浆| 他将头埋进双腿间吮小核故事| 撕开奶罩揉吮奶头免费视频| 无码精品人妻一区二区三区蜜桃 | 人妻人人澡人人添人人爽人人玩 | 成人午夜免费无码福利片| 成人毛片无码一区二区三区| 成人免费高清A级毛片| 初小VIDEOS第一次摘花| 国产大陆亚洲精品国产| 国产午夜激无码AV片在线观看| 国色天香精品一卡2卡3卡老狼| 教室停电了校草挺进我体内| 精品无码老熟妇MAGNET| 开心亚洲五月丁香五月| 免费播放AV网站的地址| 欧美老妇激情BBBWWBBW| 日本一道综合久久AⅤ免费| 十八款夜间禁用APP| 亚洲Aⅴ无码专区在线观看q| 亚洲精品国偷拍自产在线观看| 伊人色综合网一区二区三区| AⅤ中文字幕不卡在线无码| 把腿张开让老子臊烂你的视频| 福利 无码 三级 视频| 国产一卡2卡3卡4卡网站免费| 精品久久久久久中文字幕无码VR| 老头霸占人妻中文字幕| 日本XXXX裸体XXXX免费| 无码人妻精品一区二区三区99不卡| 亚洲VA国产VA天堂VA久久| 在线看片无码永久免费视频| 拔萝卜日本视频在线观看免费 | 玩丰满少妇XXXXXⅩ性麻| 亚洲AV永久无码精品一区二区| 野花香电视剧全集免费观看 | 国产精品18HDXXXⅩ| 娇妻宾馆被三根粗大的夹击 | 男人躁女人到高潮视频| 日本成熟人妻HD| 亚洲 欧美 变态 另类 综合| 亚洲一区二区三区蜜桃| 99久久无色码中文字幕人妻| 国产A三级久久精品| 娇喘潮喷抽搐高潮在线观看视频 | 狠狠爱ADY亚洲色| 免费少妇A级毛片| 日文中字乱码一二三区别在| 亚洲AV无码成人精品区明星换面 | 日韩在线看片免费人成视频播放| 亚洲AV成人片无码www妖精| 婬乱丰满熟妇XXXXⅩ性| 成人午夜又粗又硬又长| 加勒比色综合久久久久久久久| 欧美成人精品视频一区二区三区| 熟妇人妻不卡无码一区| 亚洲色WWW永久网站| 啊轻点灬大JI巴太粗太长了在线 | 日韩精品内射视频免费观看| 亚洲AV无码专区在线播放| 777久久精品一区二区三区无码| 国产成人AV片无码免费| 久久综合九色综合97欧美| 日韩精品一区二区三区在线观看L 日韩精品一区二区三区在线观看 日韩精品一区二区三区影院 | 波多野结衣高潮AV在线播放| 国产午夜亚洲精品理论片不卡| 麻花传媒免费网站在线观看| 淑芬二腿间又痒了| 夜夜嗨AV熟妇人妻涩爱AV| 成年女人A级毛片免费观看| 国精品无码一区二区三区左线| 女厕脱裤撒尿大全视频| 无码人妻精品一区二区蜜桃视频 | 噜噜私人影片在线看片| 天堂8在线天堂资源BT| 尤物193在线人妻精品免费| 国产Chinese男男视频| 老少配XXOO老少配| 我的娇妻QUEEN| 中文字日产幕码三区的做法大全| 国产精华液一二三区别 | 欧美疯狂做受XXXX高潮小说| 亚洲A∨精品无码一区二区| CHINESE熟女老女人HD视| 黑人刚破完处就三P| 日本喷奶水中文字幕视频| 亚洲色成人网站WWW永久下载 | 欧美人与动牲交片免费| 亚洲国产成人久久精品99| 博士用模型查出医院多收10万| 久久国产精品成人免费| 少妇内射高潮福利炮| 18禁美女黄网站色大片免费看| 国产精品亚洲污污网站入口 | 人妻丰满熟妇AV无码区免| 亚洲卡1卡2乱码新区仙踪| 国产 中文 制服丝袜 另类| 男女后进式猛烈XX00动态图| 亚洲AV永久天码精品天堂DL| 成人网站WWW污污污网站| 乱码人妻Av一区二区三区| 亚洲A∨无码男人的天堂| 成在人线AV无码免观看麻豆| 免费无人区一码二码乱码| 亚洲国产成人综合在线不卡| 国产69精品久久久久观看软件| 男女无遮挡猛进猛出免费视频| 亚洲ΑV久久久噜噜噜噜噜| 高清一区二区三区日本久| 欧美人与鲁交大毛片免费| 亚洲综合久久成人AV| 国产日产欧产精品品不卡| 日韩精品无码AV中文无码版| 祖母和おばあちゃん的区别| 精品无码国产一区二区三区麻豆| 乌克兰性猛交ⅩXXX乱大交| 部长来家里喝酒日剧叫什么| 免费看老外操B视频| 亚洲欧美偷拍另类A∨色屁股| 国产精品日韩专区第一页| 人与各种动ZZZ0O0OⅩⅩX| 自偷自拍亚洲综合精品麻豆| 久草日B视频一二三区| 羞羞麻豆国产精品1区2区3区 | 无人区一线二线三线乱码| 成人无码H动漫在线网站樱花| 哦┅┅快┅┅用力啊┅警花少妇 | 中国CHINESE老熟女| 九九九精品成人免费视频小说| 无遮挡又色又刺激的视频黄| 成人永久免费福利视频免费| 欧美最猛黑人XXXⅩ猛男野外| 中文字幕AV一区中文字幕天堂| 久久久久国色AV免费看图片| 国产一区二区三区无码免费 | 成人午夜精品无码区| 女人来高潮水多视频| 在线观看免费A∨网站| 中国熟妇毛多多裸交视频| ZOOM动物高清视频| 久久久久久久99精品免费观看 | 我一边做饭一边被躁了怎么回事| CHINESE激烈高潮HD| 妺妺窝人体色www聚色窝图| 野花日本中文免费完整版4| 精品VPSWINDOWS妇女| 亚洲AV色先锋资源电影网站| 国产精品免费一区二区三区四区| 少妇无码AV无码专区线| 才摸两下小奶头就受不了了| 欧美无遮挡很黄裸交视频| 7777色情XXXX欧美| 欧美 日韩 国产 成人 在线观看 | 天美传媒自制剧免费观看| 成人欧美一区二区三区黑人| 人妻洗澡被强公日日澡| 被CAO的合不拢腿| 清一区二区国产好的精华液| XXXX内射美国老太太| 人妻 丝袜美腿 中文字幕| 锕锕锕锕锕锕~好湿WWW| 人人妻人人澡人人爽人人精直播| 把腿张开老子CAO烂你| 日本人妻丰满大屁股a v|